Detractio aenea est cuprum cum stanno, aluminio, et vestigatione elementorum ut materiarum rudium, per processus per ingos, calido convolutus, frigidus involutus, curatio caloris, superficies purgatio, sectio, consummatio et sarcina, materia magna cedunt vires, lassitudo vires, elasticae proprietates. et excellens flexionis formabilitas.In CPU nervum, currus terminales, telephonum mobile keypad, electricum et alios electronicos connexiones summus technicorum usus est.
Pelagus Technical Parametri
3-1 Chemical Compositio
Nomen | Admisce No. | Compositio chemica (%.Max.) | ||||||||
Sn | Al | Zn | Ni | Fe | Pb | P | Cu | immunditia | ||
plumbum aereum | QSn4-0.3 | 3.5-4.9 | --- | 0.30 | 0.2 | 0.10 | 0.05 | 0.03-0.35 | Rem | 0.2 |
QSn4-3 | 3.5-4.5 | 0.002 | 2.7-3.3 | 0.2 | 0.05 | 0.02 | 0.03-0.35 | Rem | 0.2 | |
QSn6.5-0.1 | 6.0-7.0 | 0.002 | 0.3 | 0.2 | 0.02 | 0.02 | 0.1-0.25 | Rem | 0.1 | |
QSn8-0.3 | 7.0-9.0 | ------ | 0.2 | 0.2 | 0.10 | 0.05 | 0.03-0.35 | Rem | 0.1 | |
Aluminium Bronze | QAl5 | 0.1 | 4.0-6.0 | 0.5 | 0.5 | 0.5 | 0.03 | 0.01 | Rem | 1.6 |
QAl7 | ----- | 6.0-8.5 | 0.2 | 0.5 | 0.5 | 0.02 | ------ | Rem | ------ | |
QAl9-2 | 0.1 | 8.0-10.0 | 1.0 | 0.5 | 0.5 | 0.03 | 0.01 | Rem | 1.7 |
Nomen | Admisce No. | Compositio chemica (%.Max.) | |||||||||
Be | Al | Si | Ni | Fe | Pb | Ti | Co | Cu | impudicitia | ||
Beryllium Bronze | QBe2 | 1.8-2.1 | 0.15 | 0.15 | 0.2-0.4 | 0.15 | 0.005 | --- | --- | Rem | 0.5 |
QBe1.9 | 1.85-2.1 | 0.15 | 0.15 | 0.2-0.4 | 0.15 | 0.005 | 0.10-0.25 | --- | Rem | 0.5 | |
QBe1.7 | 1.6-1.85 | 0.15 | 0.15 | 0.2-0.4 | 0.15 | 0.005 | 0.10-0.25 | --- | Rem | 0.5 | |
QBe0.6-2.5 | 0.4-0.7 | 0.20 | 0.20 | ------ | 0.10 | --- | --- | 2.4-2.7 | Rem | --- | |
QBe0.4-1.8 | 0.2-0.6 | 0.20 | 0.20 | 1.4-2.2 | 0.10 | --- | --- | 0.30 | Rem | --- | |
QBe0.3-1.5 | 0.25-0.5 | 0.20 | 0.20 | ------ | 0.10 | --- | --- | 1.4-1.7 | Rem | --- |
3-2 Admisce Tabula
Nomen | China | ISO | ASTM | JIS |
plumbum aereum | QSn4-0.3 | CuSn4 | C51100 | C5101 |
QSn4-3 | CuSn4Zn2 | --- | --- | |
QSn6.5-0.1 | CuSn6 | C51900 | C5191 | |
QSn8-0.3 | CuSn8 | C52100 | C5210 | |
Aluminium Bronze | QAl5 | CuAl5 | C60600 | ------ |
QAl7 | CuAl7 | C61000 | ------ | |
QAl9-2 | CuAl9Mn2 | ------ | ------ | |
Beryllium Bronze | QBe2 | CuBe2 | C17200 | C1720 |
QBe1.9 | ------ | ------ | ------ | |
QBe1.7 | CuBe1.7 | C17000 | C1700 | |
QBe0.6-2.5 | ------ | C17500 | C1750 | |
QBe0.4-1.8 | ------ | C17510 | C1751 | |
QBe0.3-1.5 | ------ | C17600 | C1760 |
Pelagus Technical Parametri
3-3-1Specification Unit: mm
Nomen | Alloy No. (Sina) | Ingenium | Magnitudo (mm) | |
Crassitudo | Latitudo | |||
Tin Bronze Strip | QSn4-3 QSn4-0.3 QSn6.5-0.1QSn8-0.3 | O 1/2H H EH | 0.12~2.0 | ≤600 |
OH EH | ||||
Aluminium Bronze Strip | QA15 QA17 QA19-2 | O | 0.2~1.2 | 80~300 |
1/2H H | ||||
OH EH | 0.2~1.2 | 80~300 | ||
Beryllium Bronze Strip | QBe2 QBe1.9 QBe1.7 QBe0.6-2.5 QBe0.4-1.8 QBe0.3-1.5 | O | 0.05-1.5 | 10~340 |
H |
Ingenium Mark:O.Mollis, 1/4H.1/4 Hard;1/2H.1/2 Ferreus, H.Durum: EH.Ultrahard.
3-3-2 Tolerantia Unit: mm
Crassitudo | Latitudo | |||
Crassitudo Sine Deviation ± | Latitudo sine declinatio ± | |||
<300 | <600 | <400 | <600 | |
0.05~0.1 | 0.005 | ----- | 0.2 | ----- |
0.1~0.3 | 0.008 | 0.014 | 0.3 | 0.4 |
0.3~0.5 | 0.014 | 0.018 | 0.3 | 0.5 |
0.5~0.8 | 0.018 | 0.030 | 0.3 | 0.5 |
0.8~1.2 | 0.030 | 0.041 | 0.4 | 0.6 |
3-3-3 Mechanica euismod:
Ingenium | Distrahentes fortitudo N/mm2 | Prolongatio ≥% | duritia HV | |
M | (O) | ≥295 | 40 | ------ |
Y4 | (1/4H) | 390-510 | 35 | 100-160 |
Y2 | (1/2H) | 440-570 | 10 | 160-205 |
Y | (H) | 540-690 | 8 | 180-230 |
T | (EH) | ≥640 | 5 | ≥200 |
Ingenium Mark:O.Mollis, 1/4H.1/4 Hard;1/2H.1/2 Ferreus, H.Durum: EH.Ultrahard.